ELECTRICAL
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Dielectric Strength, in oil, 1.6 mm | 22.4 | kV/mm | ASTM D149 |
Dissipation Factor, 1 MHz | 0.017 | - | ASTM D150 |
NORYL GTX951W resin is a non-reinforced alloy of Polyphenylene Ether (PPE) + Polyamide (PA). This injection moldable grade exhibits high heat resistance, excellent chemical resistance, high melt flow, and added mold release. NORYL GTX951W resin was designed for automotive under-the-hood applications such as power distribution boxes, relay boxes, and junction boxes.
All colors are customizable. Refer our ColorXpress tool to check color availability
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Dielectric Strength, in oil, 1.6 mm | 22.4 | kV/mm | ASTM D149 |
Dissipation Factor, 1 MHz | 0.017 | - | ASTM D150 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
UL Yellow Card Link | View | - | - |
UL Recognized, 94HB Flame Class Rating | 1.2 | mm | UL 94 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Izod Impact, notched, 23°C | 211 | J/m | ASTM D256 |
Izod Impact, notched, -30°C | 100 | J/m | ASTM D256 |
Instrumented Dart Impact Energy @ peak, 23°C | 48 | J | ASTM D3763 |
Instrumented Dart Impact Energy @ peak, -30°C | 32 | J | ASTM D3763 |
Izod Impact, notched 63.5*12.7*3.2, 23°C | 13 | kJ/m² | ISO 180/4A |
Izod Impact, notched 63.5*12.7*3.2, -30°C | 8 | kJ/m² | ISO 180/4A |
Charpy Impact, notched, 23°C | 21 | kJ/m² | ISO 179/2C |
Charpy Impact, notched, -20°C | 10 | kJ/m² | ISO 179/2C |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Drying Temperature | 95 - 105 | °C | |
Drying Time | 3 - 4 | Hrs | |
Drying Time (Cumulative) | 8 | Hrs | |
Maximum Moisture Content | 0.07 | % | |
Minimum Moisture Content | 0.02 | % | |
Melt Temperature | 270 - 295 | °C | |
Nozzle Temperature | 270 - 295 | °C | |
Front - Zone 3 Temperature | 265 - 295 | °C | |
Middle - Zone 2 Temperature | 260 - 295 | °C | |
Rear - Zone 1 Temperature | 255 - 295 | °C | |
Mold Temperature | 65 - 95 | °C | |
Back Pressure | 0.3 - 1.4 | MPa | |
Screw Speed | 20 - 100 | rpm | |
Shot to Cylinder Size | 30 - 50 | % | |
Vent Depth | 0.013 - 0.038 | mm |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Tensile Stress, yld, Type I, 50 mm/min | 65 | MPa | ASTM D638 |
Tensile Stress, brk, Type I, 50 mm/min | 57 | MPa | ASTM D638 |
Tensile Strain, yld, Type I, 50 mm/min | 5 | % | ASTM D638 |
Tensile Strain, brk, Type I, 50 mm/min | 55 | % | ASTM D638 |
Tensile Modulus, 50 mm/min | 2250 | MPa | ASTM D638 |
Flexural Stress, brk, 2.6 mm/min, 100 mm span | 100 | MPa | ASTM D790 |
Flexural Modulus, 2.6 mm/min, 100 mm span | 2550 | MPa | ASTM D790 |
Tensile Stress, yield, 50 mm/min | 66 | MPa | ISO 527 |
Tensile Strain, break, 50 mm/min | 51 | % | ISO 527 |
Flexural Stress, break, 2 mm/min | 98 | MPa | ISO 178 |
Flexural Modulus, 2 mm/min | 2370 | MPa | ISO 178 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Specific Gravity | 1.1 | - | ASTM D792 |
Mold Shrinkage, flow, 24 hrs | 1.4 - 1.7 | % | ASTM D955 |
Mold Shrinkage, xflow, 24 hrs | 1.2 - 1.5 | % | ASTM D955 |
Melt Flow Rate, 280°C/2.16 kgf | 24 | g/10 min | ASTM D1238 |
Melt Flow Rate, 280°C/5.0 kgf | 65 | g/10 min | ASTM D1238 |
Water Absorption, (23°C/24hrs) | 1.99 | % | ISO 62-1 |
Moisture Absorption, (23°C/50% RH/Equilibrium) | 0.39 | % | ISO 62-4 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
HDT, 0.45 MPa, 6.4 mm, unannealed | 195 | °C | ASTM D648 |
CTE, -40°C to 40°C, flow | 9.E-05 | 1/°C | ASTM E831 |
CTE, -40°C to 40°C, xflow | 8.5E-05 | 1/°C | ASTM E831 |
CTE, 60°C to 138°C, flow | 1.67E-04 | 1/°C | ASTM E831 |
CTE, 60°C to 138°C, xflow | 1.53E-04 | 1/°C | ASTM E831 |
HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm | 181 | °C | ISO 75/Be |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Dielectric Strength, in oil, 1.6 mm | 22.4 | kV/mm | ASTM D149 |
Dissipation Factor, 1 MHz | 0.017 | - | ASTM D150 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
UL Yellow Card Link | View | - | - |
UL Recognized, 94HB Flame Class Rating | 1.2 | mm | UL 94 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Izod Impact, notched, 23°C | 211 | J/m | ASTM D256 |
Izod Impact, notched, -30°C | 100 | J/m | ASTM D256 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Drying Temperature | 100 - 120 | °C | |
Drying Time | 2 - 3 | Hrs | |
Maximum Moisture Content | 0.07 | % | |
Melt Temperature | 280 - 310 | °C | |
Nozzle Temperature | 270 - 300 | °C | |
Front - Zone 3 Temperature | 280 - 300 | °C | |
Middle - Zone 2 Temperature | 270 - 290 | °C | |
Rear - Zone 1 Temperature | 260 - 280 | °C | |
Hopper Temperature | 60 - 80 | °C | |
Mold Temperature | 80 - 120 | °C |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Tensile Stress, yld, Type I, 50 mm/min | 65 | MPa | ASTM D638 |
Tensile Strain, brk, Type I, 50 mm/min | 55 | % | ASTM D638 |
Flexural Stress, yld, 2.6 mm/min, 100 mm span | 100 | MPa | ASTM D790 |
Flexural Modulus, 2.6 mm/min, 100 mm span | 2450 | MPa | ASTM D790 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Specific Gravity | 1.1 | - | ASTM D792 |
Melt Flow Rate, 280°C/2.16 kgf | 24 | g/10 min | ASTM D1238 |
Melt Flow Rate, 280°C/5.0 kgf | 65 | g/10 min | ASTM D1238 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
HDT, 0.45 MPa, 6.4 mm, unannealed | 195 | °C | ASTM D648 |
CTE, -40°C to 40°C, flow | 9.E-05 | 1/°C | ASTM E831 |
CTE, -40°C to 40°C, xflow | 8.5E-05 | 1/°C | ASTM E831 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Dielectric Strength, in oil, 1.6 mm | 22.4 | kV/mm | ASTM D149 |
Dissipation Factor, 1 MHz | 0.017 | - | ASTM D150 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Izod Impact, notched, 23°C | 211 | J/m | ASTM D256 |
Izod Impact, notched, -30°C | 100 | J/m | ASTM D256 |
Instrumented Dart Impact Energy @ peak, 23°C | 48 | J | ASTM D3763 |
Instrumented Dart Impact Energy @ peak, -30°C | 32 | J | ASTM D3763 |
Izod Impact, notched 63.5*12.7*3.2, 23°C | 13 | kJ/m² | ISO 180/4A |
Izod Impact, notched 63.5*12.7*3.2, -30°C | 8 | kJ/m² | ISO 180/4A |
Charpy Impact, notched, 23°C | 21 | kJ/m² | ISO 179/2C |
Charpy Impact, notched, -20°C | 10 | kJ/m² | ISO 179/2C |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Drying Temperature | 95 - 105 | °C | |
Drying Time | 3 - 4 | Hrs | |
Drying Time (Cumulative) | 8 | Hrs | |
Maximum Moisture Content | 0.07 | % | |
Minimum Moisture Content | 0.02 | % | |
Melt Temperature | 270 - 295 | °C | |
Nozzle Temperature | 270 - 295 | °C | |
Front - Zone 3 Temperature | 265 - 295 | °C | |
Middle - Zone 2 Temperature | 260 - 295 | °C | |
Rear - Zone 1 Temperature | 255 - 295 | °C | |
Mold Temperature | 65 - 95 | °C | |
Back Pressure | 0.3 - 1.4 | MPa | |
Screw Speed | 20 - 100 | rpm | |
Shot to Cylinder Size | 30 - 50 | % | |
Vent Depth | 0.013 - 0.038 | mm |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Tensile Stress, yld, Type I, 50 mm/min | 65 | MPa | ASTM D638 |
Tensile Stress, brk, Type I, 50 mm/min | 57 | MPa | ASTM D638 |
Tensile Strain, yld, Type I, 50 mm/min | 5 | % | ASTM D638 |
Tensile Strain, brk, Type I, 50 mm/min | 55 | % | ASTM D638 |
Tensile Modulus, 50 mm/min | 2250 | MPa | ASTM D638 |
Flexural Stress, brk, 2.6 mm/min, 100 mm span | 100 | MPa | ASTM D790 |
Flexural Modulus, 2.6 mm/min, 100 mm span | 2550 | MPa | ASTM D790 |
Tensile Stress, yield, 50 mm/min | 66 | MPa | ISO 527 |
Tensile Strain, break, 50 mm/min | 51 | % | ISO 527 |
Flexural Stress, break, 2 mm/min | 98 | MPa | ISO 178 |
Flexural Modulus, 2 mm/min | 2370 | MPa | ISO 178 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Specific Gravity | 1.1 | - | ASTM D792 |
Mold Shrinkage, flow, 24 hrs | 1.4 - 1.7 | % | ASTM D955 |
Mold Shrinkage, xflow, 24 hrs | 1.2 - 1.5 | % | ASTM D955 |
Melt Flow Rate, 280°C/2.16 kgf | 24 | g/10 min | ASTM D1238 |
Melt Flow Rate, 280°C/5.0 kgf | 65 | g/10 min | ASTM D1238 |
Water Absorption, (23°C/24hrs) | 1.99 | % | ISO 62-1 |
Moisture Absorption, (23°C/50% RH/Equilibrium) | 0.39 | % | ISO 62-4 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
HDT, 0.45 MPa, 6.4 mm, unannealed | 195 | °C | ASTM D648 |
CTE, -40°C to 40°C, flow | 9.E-05 | 1/°C | ASTM E831 |
CTE, -40°C to 40°C, xflow | 8.5E-05 | 1/°C | ASTM E831 |
CTE, 60°C to 138°C, flow | 1.67E-04 | 1/°C | ASTM E831 |
CTE, 60°C to 138°C, xflow | 1.53E-04 | 1/°C | ASTM E831 |
HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm | 181 | °C | ISO 75/Be |