ELECTRICAL
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Surface Resistivity | 1.E+16 | Ω | ASTM D257 |
Relative Permittivity, 50/60 Hz | 2.93 | - | ASTM D150 |
Arc Resistance, Tungsten {PLC} | 6 | PLC Code | ASTM D495 |
NORYL GFN3L resin is a 30% glass fiber reinforced blend of polyphenylene ether (PPE) + polystyrene (PS). This injection moldable grade exhibits improved hydrolytic stability along with very low moisture absorption, high strength, Low warp, low specific gravity, and excellent dimensional stability. NORYL GFN3L carries a UL HB flame rating and is an excellent candidate for a variety of indoor and outdoor applications including construction, electrical components + displays, lawn and garden equipment. *See NORYL GFN3F resin for FDA food compliant / NSF version
All colors are customizable. Refer our ColorXpress tool to check color availability
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Surface Resistivity | 1.E+16 | Ω | ASTM D257 |
Relative Permittivity, 50/60 Hz | 2.93 | - | ASTM D150 |
Arc Resistance, Tungsten {PLC} | 6 | PLC Code | ASTM D495 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
UL Yellow Card Link | View | - | - |
UL Recognized, 94HB Flame Class Rating | ≥1.5 | mm | UL 94 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Izod Impact, notched, 23°C | 127 | J/m | ASTM D256 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Drying Temperature | 110 - 120 | °C | |
Drying Time | 3 - 4 | Hrs | |
Drying Time (Cumulative) | 8 | Hrs | |
Maximum Moisture Content | 0.02 | % | |
Melt Temperature | 300 - 325 | °C | |
Nozzle Temperature | 300 - 325 | °C | |
Front - Zone 3 Temperature | 290 - 325 | °C | |
Middle - Zone 2 Temperature | 275 - 320 | °C | |
Rear - Zone 1 Temperature | 265 - 315 | °C | |
Mold Temperature | 80 - 110 | °C | |
Back Pressure | 0.3 - 0.7 | MPa | |
Screw Speed | 20 - 100 | rpm |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Tensile Stress, yield | 117 | MPa | SABIC - Japan Method |
Tensile Strain, break | 8 - 10 | % | SABIC - Japan Method |
Flexural Stress | 159 | MPa | ASTM D790 |
Flexural Modulus | 7440 | MPa | ASTM D790 |
Hardness, Rockwell R | 121 | - | ASTM D785 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
Specific Gravity | 1.31 | - | ASTM D792 |
Water Absorption, (23°C/24hrs) | 0.06 | % | ASTM D570 |
Mold Shrinkage, flow, 3.2 mm | 0.2 - 0.3 | % | SABIC method |
Melt Flow Rate, 300°C/5.0 kgf | 8.3 | g/10 min | ASTM D1238 |
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS |
---|---|---|---|
HDT, 1.82 MPa, 6.4 mm, unannealed | 140 | °C | ASTM D648 |
CTE, -30°C to 30°C | 0.00002 - 0.000043 | 1/°C | TMA |